Test procedures for rubber cushioning pads

Mar 09, 2026

Leave a message

1. Add refrigerant (usually solid carbon dioxide or liquid nitrogen) to a cryogenic flask containing the heat transfer medium (generally ethanol), and stir mechanically or manually to ensure uniform temperature. Adjust the temperature to 4-5°C lower than the test temperature.

 

2. Immerse the instrument's compression device in the cryogenic flask and freeze for at least 15 minutes.

 

3. Remove the instrument's compression device from the cryogenic flask, and quickly calibrate the dial indicator zero using a 10.0±0.1mm metal gauge block.

 

4. Adjust the heat transfer medium temperature to 1-2°C lower than the test temperature. Place the rubber pad sample between the cooled instrument's indenter and compression platform. Within 5 seconds, measure the original height h<sub>o</sub> of the rubber pad sample. Then, quickly compress the rubber pad sample to 80% of its original height and record the original height h<sub>o</sub> and the compressed height h<sub>1</sub>.

 

5. Place the instrument's compression device, along with the compressed rubber pad sample, into the cryogenic flask and freeze for 5.0 ± 0.1 min. Release the handwheel within 10 seconds to remove the compression load, allowing the rubber pad sample to recover in the cryogenic flask for 3 ± 0.1 min. Read and record the recovery height h2 from the dial gauge.

 

6. Remove the compression device from the cryogenic flask and take out the rubber pad sample.

 

7. Prepare another rubber pad sample following steps 6.4-6.6.

 

8. During the rubber pad test, temperature fluctuations should not exceed 1°C. Stirring and the addition of solid carbon dioxide are prohibited.

 

9. During the rubber pad test, the thermometer bulb should be at the same horizontal level as the rubber pad sample, and the penetration depth of the rubber pad sample should not be less than 75 mm.

 

10. After the rubber pad test, wipe the instrument's indenter and compression platform dry.