NBR vs. FKM Rubber: Key Differences in Oil and Fuel Resistance

Nov 16, 2026

Leave a message

NBR and FKM are two commonly specified elastomers for rubber seals exposed to oils, fuels, and industrial fluids. Both materials are used in O-rings, gaskets, oil seals, and molded rubber components, but their resistance varies with fluid composition, temperature, exposure duration, and rubber formulation. For equipment manufacturers and industrial procurement teams, selecting between NBR and FKM requires more than comparing general material properties. The actual operating conditions and sealing structure must also be considered.

 

 

What Are the Main Differences Between NBR and FKM Rubber?

NBR, or nitrile butadiene rubber, is a copolymer of acrylonitrile and butadiene. Its acrylonitrile content influences oil resistance, while the butadiene component contributes to elasticity and low-temperature flexibility. Different NBR grades are formulated with different acrylonitrile levels to balance these properties.

FKM is a fluorocarbon elastomer containing a high proportion of fluorine. Its molecular structure provides resistance to many oils, fuels, and chemical substances, particularly under elevated temperatures. FKM compounds are commonly selected for sealing components operating in environments where both fluid exposure and heat contribute to material degradation.

The main distinction is that NBR is frequently selected for general oil-contact applications, while FKM is considered when higher temperature resistance and broader chemical compatibility are required.

FKM Viton O Ring
FKM Viton O Ring
 NBR Cured O Rings
 
NBR Cured O Rings

 

How Does NBR Perform in Oil and Fuel Environments?

NBR provides resistance to many petroleum-based oils, lubricants, hydraulic fluids, and fuels. Its oil resistance is strongly related to acrylonitrile content. Higher acrylonitrile grades generally provide better resistance to hydrocarbon oils and fuels but may have reduced low-temperature flexibility.

NBR is used in applications such as:

  • Hydraulic cylinder seals exposed to mineral-based hydraulic oils.
  • Oil seals in pumps, gearboxes, and rotating machinery.
  • O-rings installed in fuel handling equipment.
  • Gaskets used in engine and industrial machinery assemblies.
  • Rubber components exposed to lubricating oils and greases.

However, NBR does not provide the same level of resistance to every fuel formulation. Aromatic hydrocarbons, certain additives, and oxygenated fuel components can affect swelling and mechanical properties. Compatibility should therefore be evaluated against the actual fluid rather than relying only on the general term "fuel."

 

Why Does FKM Offer Better Resistance in Many Fuel Applications?

FKM has a fluorinated polymer structure that limits interaction with many hydrocarbon-based fluids. This characteristic helps maintain dimensional stability and mechanical properties when seals are exposed to oils, fuels, and elevated temperatures.

Compared with standard NBR compounds, FKM generally provides better resistance to:

  • High-temperature engine oils and lubricants.
  • Many petroleum-based fuels.
  • Diesel and gasoline under specified operating conditions.
  • Certain hydraulic fluids and industrial chemicals.
  • Oil exposure combined with elevated operating temperatures.

However, FKM is not universally resistant to all chemicals. Some ketones, esters, amines, and other specific chemical groups can cause incompatibility depending on the FKM formulation. Fuel blends containing alcohols or other oxygenated components also require careful material verification.

 

NBR vs. FKM: Oil and Fuel Resistance Comparison

The following table summarizes their general performance characteristics. Actual results depend on compound formulation, fluid composition, temperature, and exposure time.

Comparison Factor

NBR Rubber

FKM Rubber

Petroleum-based oil resistance

Good to very good, depending on grade

Generally very good

Gasoline resistance

Suitable for many formulations

Generally very good, subject to fuel composition

Diesel resistance

Commonly used

Generally very good

High-temperature oil exposure

More limited

Better suited to elevated temperatures

Aromatic fuel components

Resistance varies by grade

Generally better resistance

Low-temperature flexibility

Often better, depending on grade

Can be more limited in standard formulations

Chemical resistance

Moderate to good for selected fluids

Broad resistance, with specific chemical limitations

Typical sealing applications

Hydraulic seals, oil seals, general-purpose O-rings

Engine seals, fuel system seals, high-temperature oil seals

This comparison should be used for preliminary material selection rather than as a substitute for fluid compatibility testing.

 

How Do Acrylonitrile Content and FKM Formulation Affect Performance?

Not all NBR compounds have identical oil resistance. Acrylonitrile content is an important factor in determining the balance between oil resistance and flexibility. Higher acrylonitrile content generally reduces oil swelling but can increase stiffness at low temperatures. Lower acrylonitrile grades provide better flexibility in colder environments but may experience greater volume changes when exposed to certain oils.

FKM also includes different polymer and curing systems. Fluorine content, polymer composition, and compound additives influence resistance to specific fuels, chemicals, and temperature conditions. A standard FKM compound should not automatically be treated as suitable for every fuel system.

When comparing materials, technical specifications should identify the actual compound grade rather than simply stating NBR or FKM.

 

What Temperature Conditions Should Be Considered?

Temperature affects both the chemical resistance and mechanical behavior of rubber seals. As operating temperature increases, fluid penetration and chemical reactions can accelerate. Rubber may gradually harden, soften, lose elasticity, or develop cracks.

NBR is commonly used in moderate-temperature oil-contact applications. Its temperature capability depends on the specific compound, with conventional grades generally offering a more limited high-temperature range than FKM.

FKM is frequently selected for higher-temperature sealing environments, including engine compartments, industrial pumps, and fuel-handling equipment. It can retain useful sealing properties under heat exposure that would accelerate degradation in many standard NBR compounds.

Low-temperature operation requires separate consideration. Standard FKM grades may become less flexible in cold environments, while specialized low-temperature formulations are available. The minimum operating temperature should therefore be confirmed for the selected compound.

 

Which Material Is More Suitable for Different Industrial Applications?

The choice depends on the fluid, temperature, pressure, and movement of the sealing component.

Application

Common Material Consideration

Main Selection Factor

Hydraulic systems using mineral oil

NBR

Oil compatibility and pressure conditions

Industrial gearboxes

NBR or FKM

Oil temperature and maintenance interval

Automotive fuel systems

NBR or FKM

Fuel formulation and operating temperature

Engine oil sealing

NBR or FKM

Continuous heat and oil exposure

High-temperature fuel handling

FKM

Temperature and fuel compatibility

General-purpose oil seals

NBR

Cost, flexibility, and oil resistance

Chemical processing equipment

FKM or another specialized compound

Specific chemical compatibility

For example, an NBR O-ring in a standard hydraulic circuit may provide the required sealing performance when the fluid and temperature are within the compound's operating limits. A seal exposed to hot engine oil or a more demanding fuel environment may require FKM to reduce the risk of swelling and thermal degradation.

 

How Does Fluid Exposure Cause Rubber Seal Failure?

Oil and fuel exposure can change rubber properties through absorption, extraction, and chemical degradation. These changes affect the seal's dimensions and ability to maintain contact pressure.

Common failure symptoms include:

Swelling: The rubber absorbs fluid and increases in volume, potentially causing excessive compression or installation difficulties.

Hardening: Heat or chemical exposure reduces elasticity, making the seal less able to follow surface movement.

Softening: Fluid absorption or chemical interaction reduces mechanical strength and can lead to deformation.

Cracking: Thermal aging and chemical attack can create surface cracks that develop into leakage paths.

Permanent deformation: Compression set reduces the seal's ability to recover after compression, lowering contact pressure.

The same failure symptom can have different causes. For example, swelling may result from an incompatible fluid, while hardening may be associated with long-term thermal aging. Material evaluation should consider both the fluid and the mechanical conditions of the sealing position.

 

What Tests Help Evaluate NBR and FKM Compatibility?

Material selection should be supported by test data when seals operate under demanding conditions. Several standardized tests can help compare rubber compounds.

Test Method

Evaluation Purpose

Relevant Property

ASTM D471

Liquid immersion testing

Volume, mass, and hardness changes

ASTM D395

Compression set testing

Recovery after prolonged compression

ASTM D573

Heat aging in air

Changes in tensile strength, elongation, and hardness

ASTM D412

Tensile testing

Tensile strength and elongation

ASTM D2240

Durometer hardness testing

Rubber hardness

For oil and fuel applications, ASTM D471 is particularly relevant because specimens can be immersed in a specified test liquid under controlled conditions. Volume change, mass change, and hardness variation can then be compared between NBR and FKM compounds.

Testing should use the actual service fluid or a clearly identified representative test liquid. Results from one fuel formulation should not automatically be applied to another.

 

How Do Seal Design and Installation Affect Material Performance?

Even when the rubber compound is chemically compatible, an unsuitable sealing design can cause premature failure. Material selection must be coordinated with the dimensions and mechanical requirements of the component.

For O-rings, important design parameters include inner diameter, cross-sectional diameter, groove width, groove depth, and squeeze ratio. Excessive compression can accelerate permanent deformation, while insufficient compression may result in leakage.

For oil seals, the lip structure, shaft surface finish, shaft speed, and lubrication conditions influence performance. FKM may be selected for elevated-temperature oil exposure, but the lip geometry and shaft condition still need to match the operating requirements.

Gaskets require consideration of thickness, compression load, flange flatness, and surface condition. A chemically resistant material cannot compensate for uneven bolt loading or an incorrectly designed flange connection.

 

What Information Should Be Confirmed Before Ordering NBR or FKM Seals?

To reduce material and dimensional mismatches, technical specifications should include the following information:

Material: NBR, FKM, or a specific compound grade.

Fluid type: Mineral oil, hydraulic oil, gasoline, diesel, or a defined chemical mixture.

Operating temperature: Normal temperature, maximum temperature, and minimum temperature.

Pressure conditions: Working pressure and pressure fluctuations.

Seal dimensions: Inner diameter, outer diameter, cross-section, thickness, or a technical drawing.

Hardness: Required Shore A hardness, if specified.

Movement: Static sealing, reciprocating motion, or rotary motion.

Exposure conditions: Continuous immersion, intermittent contact, or occasional splashing.

Testing requirements: Fluid immersion, compression set, hardness, or other specified evaluations.

Providing this information allows the rubber compound and sealing structure to be assessed together rather than selecting material based on oil resistance alone.

 

Why Choose Haining Chaoyue Seals Co., Ltd. for Rubber Sealing Products?

Haining Chaoyue Seals Co., Ltd. focuses on rubber sealing products for industrial applications. NBR and FKM seals serve different operating requirements, so material selection needs to account for fluid compatibility, temperature, dimensions, and installation conditions.

For projects involving oil- and fuel-resistant rubber components, we focus on several practical considerations:

Material Selection: NBR and FKM have different resistance characteristics. Application details help determine which material category is more appropriate for the specified fluid and operating temperature.

Custom Dimensions: Technical drawings, samples, or dimensional specifications can be used to define O-ring sizes, gasket profiles, and other custom rubber sealing components.

Product Structure: Different sealing positions require different designs, including O-rings, gaskets, oil seals, and other molded rubber parts.

Application Requirement Review: Fluid type, pressure, temperature, hardness, and installation conditions are important details when discussing rubber seal specifications.

Order Specification Confirmation: Confirming material and dimensional requirements before ordering helps reduce misunderstandings between the product specification and the actual equipment design.

For NBR and FKM rubber seal projects, customers can provide product drawings, sample dimensions, and details about the oil or fuel environment.